首頁 > 產(chǎn)品展示 > > 其他檢測儀器 > TC-500 氧氮聯(lián)合測定儀

TC-500 氧氮聯(lián)合測定儀

簡要描述:簡單說明:TC500系列儀器質(zhì)量、性能、工藝滿足您對金屬、難熔物、其他無機材料日常生產(chǎn)中氮/氧分析的需要

  • 產(chǎn)品型號:TC-500
  • 廠商性質(zhì):生產(chǎn)廠家
  • 更新時間:2024-10-08
  • 訪  問  量:2219
詳情介紹

詳細說明:

TC500系列儀器質(zhì)量、性能、工藝滿足您對金屬、難熔物、其他無機材料日常生產(chǎn)中氮/氧分析的需要

Determination of Oxygen and Nitrogen in
Reactive/Refractory Metals and Their Alloys*
 
Approval
ASTM E-1409 Oxygen Determination in Titanium and Titanium Alloys
ASTM E-1569 Oxygen Determination in Tantalum
ASTM E-1937 Nitrogen Determination in Titanium and Titanium Alloys
 
Sample Preparation
A clean representative sample is required in order to obtain optimum results. Solid samples can be leached in suitable acid or abraded with a clean file, rinsed in acetone, and dried with warm air. Refer to ASTM methods above for further details.
 
Accessories
782-720 Crucible; 782-721 Electrode Tip; 502-344 UHP Nickel
Baskets; 501-073 Graphite; 503-032 Glass Accelerator Scoop;
501-059 Tin Capsules—for powdered samples. (Additional steps required for powdered samples are noted in parenthesis.)
 
Calibration Standard
LECO 501-320 Titanium Pin, 502-047 Zirconium Pin, NIST, or other suitable reactive/refractory metal standard.
 
Method Parameters
Analysis Parameters
Outgas Cycles                           2
Analysis Delay (seconds)             20
Analysis Comparator                 1
Analysis Type                              Auto
 
Element Parameters                  Oxygen           Nitrogen
Minimum Time (seconds)
35
55
Integration Delay (seconds)
5
15
Comparator Level (%)
1
1
 
Furnace Parameters
Furnace Control Mode             Power
Purge Time (seconds)                    15
Outgas Time (seconds)                20
Cool Time (seconds)                    5
Outgas Power (Watts)                 6300
Analyze Power (Watts)                5300
 
 
 
 
 


 

*This includes Ti, Zr, W, Mo, Ta, Nb, Hf, and their alloys.

 
TC500


 

 
Typical Results
 
 
 
Titanium Pin
Mass (g)
Oxygen (%)
Nitrogen (%)
 
0.1135
0.1808
0.0189
 
0.1133
0.1843
0.0194
 
0.1134
0.1831
0.0184
 
0.1138
0.1819
0.0188
 
0.1133
0.1821
0.0195
 
0.1131
0.1829
0.0185
 
0.1134
0.1833
0.0191
 
0.1143
0.1849
0.0194
 
0.1125
0.1837
0.0189
 
0.1072
0.1830
0.0191
 
Average
0.1830
0.0190
 
Std. Dev.
0.0012
0.0004
 
Zirconium Wire
 
Mass (g)
 
Oxygen (%)
 
Nitrogen (%)
 
0.1067
0.1246
0.0017
 
0.0978
0.1273
0.0017
 
0.1180
0.1246
0.0019
 
0.1097
0.1235
0.0014
 
0.1141
0.1272
0.0017
 
0.1017
0.1226
0.0018
 
0.1140
0.1269
0.0020
 
0.0987
0.1239
0.0020
 
0.1015
0.1233
0.0022
 
0.1197
0.1270
0.0020
 
Average
0.1251
0.0018
 
Std. Dev.
0.0018
0.0002
 
Procedure
 
 
 
1.   Determine the blank as follows:
a.   Enter the "blank" ID code with a 1.0000 g weight in the weight stack.
b.   Press the loader control switch, the sample loader will open.
c.   Place one 502-344 UHP Nickel basket into the loading head using clean tweezers.
(Place a 501-059 Tin capsule into the Nickel basket before placing it in the loading head.)
d.   Press the loader control switch, the sample loader will close and seal and the furnace electrode will open.
e.   Remove crucible from electrode tip and discard.  Clean furnace area using the appropriate brushes.  Vacuum away loose dust.
f.    Place ~0.05 g 501-073 into the bottom of a 782-720 crucible.  ~0.05 g is approximay a ¼ full
503-032 glass accelerator scoop.
g.   Place the crucible on the lower electrode.
h.   Press the loader control switch, the furnace electrode will close and the analysis sequence will start automatically.
i.    Repeat steps 1a through 1h at least four more times.
j.    Enter blank following routine outlined in operator's instruction manual.
2.   Calibrate the instrument as follows:
a.   Weigh the calibration sample. (Weigh the calibration sample into the tin capsule.)
b.   Enter the calibration sample ID code and sample weight in the weight stack.
c.   Place the calibration sample (capsule) into a nickel basket.
d.   Press the loader control switch, the sample loader will open.
e.   Carefully place the calibration sample/nickel basket (capsule) into the loading head using clean tweezers.  Make sure that the calibration sample (capsule) stays in the basket and the basket
stays upright.
f.    Press the loader control switch, the sample loader will close and seal and the furnace electrode will open.
continued on page 3


 

Procedure (continued from page 2)
g.   Remove crucible from electrode tip and discard.  Clean furnace area using the appropriate brushes.  Vacuum away loose dust.
h.   Place ~0.05 g graphite into the bottom of a crucible.
i.    Place the crucible on the lower electrode.
j.    Press the loader control switch, the furnace electrode will close and the analysis sequence will start automatically.
k.   Repeat steps 2a through 2j a minimum of three times.
l.    Complete a calibration by following the auto calibration procedure as outlined in the operator's instruction manual.
m.  Verify the calibration by analyzing the calibration sample again.  It should fall within the expected tolerances.  If not, repeat steps 2a through 2l again.
3.   Analyze the samples as follows:
a.   Weigh ~0.1 g sample. (Weigh the sample into the tin capsule.)
b.   Enter the sample ID code and sample weight in the weight stack.
c.   Place the sample (capsule) into a nickel basket.
d.   Press the loader control switch, the sample loader will open.
e.   Carefully place the sample/nickel basket (capsule) into the loading head using clean tweezers.
Make sure that the sample (capsule) stays in the basket and the basket stays upright.
f.    Press the loader control switch, the sample loader will close and seal and the furnace electrode will open.
g.   Remove crucible from electrode tip and discard.  Clean furnace area using the appropriate brushes.  Vacuum away loose dust.
h.   Place ~0.05 g graphite into the bottom of a crucible.
i.    Place the crucible on the lower electrode.
j.    Press the loader control switch, the furnace electrode will close and the analysis sequence will start automatically.
 
Theory of Operation
The TC500 is a microprocessor-based, software-controlled instrument that measures both nitrogen and oxygen in a wide variety of metals, refractories, and inorganic materials. The inert gas fusion principle is employed. A weighed sample, placed in a high-purity graphite crucible, is fused under a flowing helium gas stream at temperatures sufficient to release oxygen, nitrogen, and hydrogen. The oxygen in the
sample, combines with the carbon from the crucible to form carbon monoxide. The nitrogen present in
the sample releases as molecular nitrogen, and any hydrogen present is released as hydrogen gas. The helium carries the sample gases through heated rare earth copper oxide which converts carbon
monoxide to carbon dioxide (CO2) and hydrogen to water (H2O). The nitrogen passes through
unchanged. The gases are then passed through a CO2  infrared (IR) cell where the oxygen is measured as
CO2. CO2  and H2O are then removed by a Lecosorb/Anhydrone trap, while the nitrogen passes through
to a thermal conductivity (TC) cell for determination.


 

TC500 Flow Diagram
 
 
 
 
 

留言框

  • 產(chǎn)品:

  • 您的單位:

  • 您的姓名:

  • 聯(lián)系電話:

  • 常用郵箱:

  • 省份:

  • 詳細地址:

  • 補充說明:

  • 驗證碼:

    請輸入計算結(jié)果(填寫阿拉伯數(shù)字),如:三加四=7
技術(shù)支持:化工儀器網(wǎng)   sitemap.xml   管理登陸
©2025 版權(quán)所有:寧波市鄞州瑾瑞儀器設(shè)備有限公司   備案號:浙ICP備14028217號-3

浙公網(wǎng)安備33020402000311號

国产精品欧美一区二区三区| 无码AV久久久久久久久| 女人第一次一进去就出血| 极品少妇高潮XXXXX| 两根大肉大捧一进一出好爽视频| 国产欧美一区二区精品性色| 女人野外做爰A片妓女| 亚洲精品无码久久久久久| 免费看片的播放器| 被男人吃奶跟添下面特舒服| 性少妇FREESEXVIDEOS高清| SM女人捆绑调教网站A片软件| 宝贝把腿开大让我添添电影| 娇妻跪趴高撅肥臀出白浆| 欧亚专线S码和W码的区别| 99久久蜜AV毛片毛片正在| 无码人妻AV免费一区二区三区| 亚洲色精品三区二区一区| 中国成熟妇女毛茸茸| 欧洲熟妇色xxxxx欧美老妇伦| 国产日韩欧美一区二区三区| 亚洲成AV人片在线观看无 | 国产精品高清一区二区三区人妖| 久久精品国产久精国产| 日韩AV无码成人精品国产| FREE性玩弄妇女HD| 国偷自产AV一区二区三区动漫| 被调教的少妇雅芳1一19| 国产女人18毛片水真多18精品| 欧美成人精品第一区二区三区| 呦香8黝黝狖呦香8| 国产JAZZ亚洲护士无码| 午夜理论影院第九电影院| 国产精品无码久久久久| 夜夜性日日交XXX性HD| 美女露0的奶头无挡挡| 在线精品国产一区二区三区| 精品香蕉一区二区三区| YYY6080韩国三级理论| 国产偷抇久久精品A片69| 亚洲一区二区三区AV无码|